Run Card for cmos150 |
|
Step 30.0 |
|
|
|
|
|
|
|
Process: N+ S/D Photo: Mask N+S/D (NSD chrome-df) |
Date |
Operator |
|
|
|
|
|
|
|
Standard I-line Process with the thicker UV resist. |
February of 12th 2002 |
vorosl |
|
|
|
|
|
|
1. |
HMDS |
|
|
|
|
Program: 2 on svgcoat6 |
|
|
|
|
|
|
|
|
2. |
Spin and Soft Bake |
|
|
|
|
Program: 2 and 2 on svgcoat6 |
|
|
|
|
Photoresist: UV26-1.5 (Shipley) |
|
|
|
|
Thickness of PR: ~1.35 micron at RPM: 4000 |
|
|
|
|
|
|
|
|
3. |
Expose by ASML: energy=22 mJ/cm2 |
|
|
|
|
Mask: N+S/D |
|
|
|
4. |
Post exposure bake (Program: 2) |
|
|
|
|
(at 110 C for 90 sec) |
|
|
|
5. |
Develop (Program: 2) developer: LDD26 |
|
|
|
|
svgdev6 was down, had to hand-develop |
|
|
|
6. |
Inspect |
|
|
|
|
|
|
|
|
7. |
Descum |
|
|
|
|
This step was skipped since there was no 6” tool for it |
|
|
|
|
|
|
|
|
8. |
Hard Bake (oven) |
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|